Application Note | ElastoSens™ Bio
Quantifying the Bioprinting Workflow of TissueFab® Bioinks
Translating Thermal Conditioning and Visible-Light Crosslinking Steps into Quantitative Mechanical Information with ElastoSens™ Bio
NOTICE
This study was performed as a joint collaboration between Rheolution (QC, Canada) and MilliporeSigma (Merck – SP, Brazil).
Summary
- This application note provides quantitative mechanical context for key steps of the recommended TissueFab™ bioprinting protocol, connecting bioink preparation and thermal conditioning through printing and photocrosslinking to the final construct mechanics.
- ElastoSens™ Bio was used to quantify the mechanical transitions associated with thermal conditioning and 405 nm photocrosslinking of three TissueFab™ bioinks.
- The formulations showed distinct thermal gelation kinetics and post-crosslinking stiffnesses, demonstrating that bioink selection influences the mechanical outcome of the printing workflow.
- Light intensity and exposure duration strongly affected final G′, providing quantitative guidance for adapting photocrosslinking conditions to the desired construct mechanics.
From a Bioprinting Protocol to Measurable Material Transitions
Introduction
Successful extrusion-based 3D bioprinting requires a bioink to transition through different mechanical states: fluid enough for preparation and cartridge loading, sufficiently structured for controlled extrusion, and mechanically stable after printing. The recommended protocol provided by MilliporeSigma for TissueFab™ bioinks offers a practical baseline for this sequence, including warming the bioink to 37 °C for handling, cooling the loaded cartridge to 15–20 °C to induce gelation before printing, and exposing the printed construct to 405 nm visible light for photocrosslinking.
While these steps define the practical workflow, quantitative mechanical information can help users understand how quickly the bioink gels during cooling and how photocrosslinking conditions affect final construct stiffness. These transitions can be followed through the shear storage modulus (G′), which reflects the elastic response, and tan δ (G″/G′), which describes the balance between viscous and elastic behavior.
In this collaborative study between MilliporeSigma and Rheolution, ElastoSens™ Bio was used to monitor TissueFab™ bioinks in real time during thermal gelation and visible-light photocrosslinking. The experimental design reproduces key transitions of the recommended bioprinting workflow, providing quantitative mechanical information to support process understanding and optimization.
Replicating the Key Mechanical Steps of the Bioprinting Workflow
Material and methods
Three bioink formulations, TissueFab™ GelMA-Conductive-Vis (915963), TissueFab™ GelMA-Bone-Vis (915033), and TissueFab™ GelMA-Vis (918741) were characterized with ElastoSens™ Bio following an experimental sequence designed to reproduce the key steps of their bioprinting protocol.
Samples first underwent thermal gelation without light exposure, while G′ and tan δ were monitored continuously. At 40 min, samples were photocrosslinked with 405 nm light for 15 s at 100% intensity, and measurements were continued to quantify the resulting increase in stiffness. Thermal gelation time was identified from the characteristic maximum in tan δ, while plateau G′ was averaged between 65 and 70 min.
To evaluate the influence of photocrosslinking settings, TissueFab™ GelMA-Bone-Vis was tested at different light intensities using a fixed 15 s exposure, and TissueFab™ GelMA-Vis was tested at different exposure durations at 100% intensity.
Figure 1. Representative TissueFab™ bioinks during ElastoSens™ Bio testing (top) and after removal from the sample holders (bottom). From left to right: TissueFab™ GelMA-Vis, TissueFab™ GelMA-Bone-Vis, and TissueFab™ GelMA-Conductive-Vis.
Quantifying the Transition from Cartridge Conditioning to a Crosslinked Construct
Results and Discussion
The evolution of G′ and tan δ during the first 40 min at 20 °C revealed clear differences in thermal gelation among the three TissueFab® formulations (Fig. 1), reflecting the cartridge-cooling step performed before printing. As the bioinks progressively developed an elastic structure, the peak in tan δ was used to identify the thermal gelation time, occurring at approximately 6.5 min for TissueFab™ GelMA-Conductive-Vis, 10.3 min for TissueFab™ GelMA-Bone-Vis, and 10.4 min for TissueFab™ GelMA-Vis.
At 40 min, the samples were exposed to 405 nm light for 15 s at 100% intensity (30 mW/cm²), representing the post-deposition stabilization step. All three formulations showed a rapid increase in G′ following illumination (Fig. 1), directly quantifying the mechanical reinforcement produced by photocrosslinking. The magnitude of this response depended strongly on formulation: TissueFab™ GelMA-Conductive-Vis reached the highest plateau G′ at approximately 24.0 kPa, followed by TissueFab™ GelMA-Bone-Vis at approximately 19.2 kPa and TissueFab™ GelMA-Vis at approximately 8.3 kPa. These results demonstrate that identical photocrosslinking conditions can produce substantially different final stiffnesses, making bioink formulation an important determinant of the mechanical properties of the printed construct.
Figure 2. Quantifying thermal conditioning and photocrosslinking steps of the TissueFab™ bioprinting workflow. Evolution of the shear storage modulus (G′) and tan δ for TissueFab™ GelMA-Conductive-Vis, TissueFab™ GelMA-Bone-Vis and TissueFab™ GelMA-Vis (n=3). Samples first underwent thermal gelation at 20 °C, representing the pre-print cooling/conditioning stage, and were subsequently photocrosslinked at 40 min using 405 nm light for 15 s at 100% intensity. The right panels summarize the characteristic thermal-gelation time from tan δ and the post-crosslinking plateau G′.
Light Intensity is a Process Parameter for Tuning the Printed Construct
The MilliporeSigma workflow instructs users to crosslink the printed construct with 405 nm visible light and to adapt distance and exposure to the available light source. This makes the delivered light dose a practical processing variable. To quantify its effect, light intensity was varied while wavelength and exposure duration were maintained constant.
To evaluate the effect of light intensity, TissueFab™ GelMA-Bone-Vis samples were photocrosslinked for 15 s at 25%, 50% and 100% intensity, corresponding to approximately 8, 15 and 30 mW/cm², respectively (Fig. 2). Before light exposure, the G′ curves showed similar behavior during thermal gelation; however, following illumination at 40 min, a clear intensity-dependent response was observed, with G′ reaching approximately 3.5 kPa at 25% intensity, 9.7 kPa at 50% intensity, and 19.2 kPa at 100% intensity. These results demonstrate that increasing light intensity progressively increases the post-crosslinking stiffness of TissueFab™ GelMA-Bone-Vis over the tested range.
Therefore, transferring a printing protocol between instruments should account for the actual light delivered to the construct rather than relying on exposure time alone.
Figure 3. Effect of 405 nm light intensity on the mechanical stabilization of TissueFab™ GelMA-Bone-Vis (n=1). Following the thermal-conditioning phase, samples were exposed for 15 s using 25% (8 mW/cm²), 50% (15 mW/cm²) or 100% (30 mW/cm²) light intensity. Increasing irradiance progressively increased post-crosslinking G′, illustrating how the light-source setting can alter the mechanics of the final printed construct.
Exposure Time Provides a Second Lever for Adapting the Crosslinking Step
The MilliporeSigma protocol also identifies exposure time as a parameter that may need to be adapted to the available light source and printing configuration. The effect of this parameter was therefore quantified using TissueFab™ GelMA-Vis (Fig. 3).
Samples were photocrosslinked using 405 nm light at 100% intensity, with exposure durations of 15, 30 and 60 s. While the G′ curves showed similar behavior before photocrosslinking, clear differences emerged following light exposure, with G′ reaching approximately 8.3 kPa after 15 s, 17.3 kPa after 30 s, and 21.5 kPa after 60 s. The increase was particularly pronounced between 15 and 30 s, demonstrating that exposure duration strongly influences post-crosslinking stiffness and that relatively small changes in this parameter can substantially modify the mechanical properties of the resulting construct.
Together with the light-intensity experiment, these results highlight photocrosslinking as a critical processing step in the bioprinting workflow, since changes in irradiance, exposure duration, and source-to-construct distance can alter the effective light dose and substantially affect the final construct mechanics. This is particularly important when transferring protocols between bioprinters or external light sources, where direct mechanical characterization can help determine whether adapted crosslinking conditions achieve the desired mechanical endpoint.
Figure 4. Effect of 405 nm exposure duration on the mechanical stabilization of TissueFab™ GelMA-Vis (n=1). Following thermal conditioning, samples were exposed at 100% intensity for 15, 30 or 60 s. Increasing exposure duration resulted in progressively higher G′, quantifying the sensitivity of final construct stiffness to the duration selected for the post-print crosslinking step.
Adding Quantitative Mechanics to a Practical Bioprinting Protocol
Conclusions
The TissueFab™ protocol provides users with the practical sequence required to prepare, print and crosslink these bioinks. The present study complements that workflow by quantifying what happens mechanically during two critical transitions: thermal gelation before extrusion and photocrosslinking after deposition.
The three tested formulations displayed distinct thermal gelation behavior and substantially different mechanical properties after photocrosslinking. Under identical exposure conditions of 405 nm, 15 s and 100% intensity, TissueFab™ GelMA-Conductive-Vis produced the highest plateau G′, TissueFab™ GelMA-Bone-Vis exhibited intermediate stiffness and TissueFab® bioink produced the softest network.
The experiments further demonstrated that the final stiffness is not determined solely by formulation. For TissueFab™ GelMA-Bone-Vis, increasing light intensity from 25% to 100% produced a progressive increase in G′. Similarly, increasing the exposure duration of TissueFab™ GelMA-Conductive-Vis from 15 to 60 s substantially increased its final stiffness.
Overall, the mechanical outcome of the bioprinting workflow is governed by both bioink formulation and processing conditions: formulation influences thermal gelation and post-crosslinking stiffness, while light intensity and exposure duration provide additional control over the final construct mechanics. By quantitatively linking temperature conditioning and photocrosslinking parameters to material properties, these measurements can support process optimization, method transfer and more reproducible fabrication of 3D constructs.
Practical takeaways for the bioprinting workflow
- Preparation: warming the bioink makes it fluid for mixing and cartridge loading; this is followed by a deliberate cooling step before extrusion.
- Pre-print conditioning: thermal gelation is measurable and formulation-dependent, providing quantitative context for the cartridge-cooling step used to establish print-ready material structure.
- Printing: the thermally conditioned state precedes extrusion and helps connect temperature control with printing fidelity and shape retention.
- Post-print stabilization: 405 nm photocrosslinking produces a rapid increase in G′ and converts the deposited material into a mechanically stronger construct.
- Light-source settings matter: changing irradiance or exposure duration can substantially change the final G′, supporting the protocol recommendation to adapt crosslinking parameters to the available light source and configuration.
- Formulation matters: identical processing conditions can generate different mechanical endpoints for different TissueFab™ bioinks.
- Quantitative characterization complements the protocol: real-time viscoelastic measurements can help users connect practical processing settings with the mechanical state of the material before and after printing.
Discover how our technology non-destructively measures the viscoelastic properties of soft biomaterials and tissues using micro-volumes of samples
Related Posts
Extracellular matrix (ECM) hydrogels are biomaterials derived from native tissues after removal of cellular components through decellularization. The remaining matrix preserves key structural proteins (such as collagens, elastin, fibronectin, and laminin), proteoglycans, and glycosaminoglycans that define the biochemical and architectural identity of the source tissue. ECM is naturally produced by cells in all tissues and provides both mechanical support and biochemical signaling cues.
Superabsorbent polymer (SAP) hydrogels are three-dimensional, crosslinked polymer networks capable of absorbing and retaining extremely large amounts of water—often hundreds to thousands of times their own weight—while remaining insoluble. Their structure is based on hydrophilic polymer chains containing functional groups such as carboxylate, hydroxyl, or amide moieties, which generate strong osmotic driving forces for water uptake.
Polyacrylamide (PAM) hydrogels are synthetic, water-swollen polymer networks formed from acrylamide monomers chemically or physically crosslinked into a three-dimensional structure. Polyacrylamide itself is an organic polymer composed of repeating acrylamide subunits, and when crosslinked in aqueous environments, it forms soft, highly hydrated gels with tissue-like mechanical behavior. PAM hydrogels are entirely synthetic and industrially produced, offering high batch-to-batch reproducibility and tunable properties.
Polymethyl methacrylate (PMMA) is a synthetic, thermoplastic polymer belonging to the acrylic resin family. It is formed by the free-radical polymerization of methyl methacrylate (MMA) monomers, resulting in a linear, amorphous polymer with high optical clarity and structural rigidity. PMMA is entirely industrially produced, with MMA synthesized from petrochemical feedstocks and polymerized using controlled thermal, chemical, or photochemical initiation.